Our main products include flexible substrate coating, shielding materials, absorbing materials, precious metal slurries, and more!

banner
Current:Home >Company news >Frontier News >Magnetic medium absorbing material: Why are two different properties made for the same batch of magnetic powder
先进院(深圳)科技有限公司

Hotline:0755-22277778 Tel:0755-22277778 
Mobile:13826586185(Mr.Duan)
Fax:0755-22277776
E-mail:duanlian@xianjinyuan.cn

Frontier News

Magnetic medium absorbing material: Why are two different properties made for the same batch of magnetic powder

Time:2026-11-25Number:17

Technical Note  /  Effective Medium

Two suppliers use the same brand of magnetic powder, but the parameters of the magnetic medium absorbing wave plate they produce are twice as different: one has a μ 'of about 80, the other only has 40, and the ε' ranges from just over 10 to nearly 20. The powder is the same, the brand matches, and the report also matches——The difference lies in how the powder is organized into a "medium": how much it is filled, how flat it is pressed, how neatly it is arranged, and how thick the interface is wrapped.

This is exactly where the weight of the word 'magnetic medium' lies. It reminds us that the μ and ε on the parameter table belong to composite materials, not the materials themselves.

01Why do macro parameters need to be calculated

The working frequency of absorbing materials ranges from MHz to GHz, corresponding to free space wavelengths ranging from meters to centimeters; The size of magnetic powder particles is usually in the micrometer range, much smaller than the wavelength. This scale difference brings a convenience: it is not necessary to solve the electromagnetic field one by one, but to treat the composite material as a uniform medium and assign it an equivalent set of μ and ε. This is the starting point of the effective medium approximation.

The source of equivalent parameters can be simplified into one sentence: magnetic powder contributes to magnetic response, matrix contributes to dielectric background, and the interface and arrangement between the two determine how they "add up". Different ways of adding result in different outcomes.

02Three geometric quantities to determine macroscopic parameters

Geometric quantity The impact on μ The impact on ε
fill rate As the volume fraction increases, the return decreases as it approaches saturation Synchronous rise compresses the space for impedance matching
shape factor Flat sheet improves in-plane magnetic permeability and increases resonance frequency Increasing the interface area in flakes can easily lead to a higher ε value
Orientation degree When the orientation is consistent, the in-plane μ is high and the out of plane μ is low, with obvious anisotropy Ordered arrangement is usually easier to control than disordered aggregation

The three quantities are not independent. Increasing the filling rate to increase μ often simultaneously raises ε; flattening improves shape anisotropy and increases interface area, continuing to raise ε. Formula adjustments in engineering almost always find a balance point between these three, rather than optimizing one item separately.

Common high filling magnetic media sheets have a magnetic powder volume fraction roughly ranging from 30% to 60% (or 80% to 95% by weight), and the diameter of sheet-like particles is mostly in the range of tens of micrometers, with a thickness of about 1-3 μ m and a density of about 3.6-4.1 g/cm ³. These numbers are just common scales in the industry, and the specific formulas vary greatly.

03Mixing Rule: Why "Addition" has upper and lower bounds

There are two extremes to the simplest estimation of mixing two-phase materials: one assumes that the field is distributed parallel to the two phases, resulting in a biased result; Another assumption is that the field passes vertically through the stacked structure, resulting in a lower result. The effective parameters of real composite materials fall between these two boundaries, with the specific location determined by particle shape, distribution, and interface.

Approximate method provide Applicable impression
Parallel mixing Upper bound (high) When the sheet-like particles are highly oriented and layer by layer parallel, they approach each other
Series mixing Lower bound (lower) Rough estimation when particles are random and the interface layer is thick
Effective Media Model Between the two Taking into account the particle shape and filling rate, it is closer to the actual measurement

This also explains a common phenomenon: for the same brand of powder, the same filling rate, and different orientation processes, the measured μ 'will be significantly different. The oriented sheet is closer to the "parallel" end, the random sheet is closer to the middle, and the sample with thick interface layer will be pulled towards the "serial" end.

04Interface: The invisible layer has the greatest impact on ε

The insulation coating on the surface of magnetic powder may only be a few tens of nanometers thick, but it accounts for a very high proportion of the total interface area. The larger the aspect ratio of the sheet-like particles, the larger the interface area at the same filling rate, and the more significant the dielectric contribution brought by the coating layer.

Coating itself is necessary: it cuts off electronic conduction between particles, suppresses eddy currents, and keeps the sheet non-conductive. But it also introduces the dielectric properties of air or resin into the magnetic circuit, causing an increase in ε 'and a decrease in impedance. This is the structural contradiction between "suppressing eddy currents" and "maintaining matching" - the thicker the coating, the safer it is, but the higher the dielectric cost.

Reunion is another pathway. After the particles aggregate into clusters, they come into contact with each other, which is equivalent to the appearance of local conductors, and both the ε 'and loss will be significantly increased; If the size of the cluster exceeds the skin depth of the frequency band, the eddy current loss increases accordingly. Macroscopically, this batch has a particularly high ε, while microscopically, there is a problem with the consistency of the dispersion process.

Remember one sentenceMagnetic powder determines how strong it can be, while interface and arrangement determine how much it actually is.

05A physical constraint: μ 'and μ' cannot be specified separately

The electromagnetic parameters of materials are subject to causal constraints: the real and imaginary parts are not two independent numbers that can be combined arbitrarily, they are bound to each other through an integral relationship. The intuitive meaning is that in order to obtain loss in a certain frequency band, one must pay the cost of dispersion in adjacent frequency bands; It is impossible to produce materials with high losses but completely flat real parts.

This constraint provides a practical validation tool. When a magnetic spectrum data shows a significant peak in a certain frequency band μ ", but there is no change in μ 'at that location, there is a high probability that there is a problem with the data: either parasitic losses are tested, or the curve has been smoothed. On the contrary, if μ 'exhibits a typical decreasing transition near the resonance peak, the data is usually more reliable.

It is not an exact criterion, but it is sufficient to screen out reports that are clearly non physical. For procurement, this is faster than checking values point by point.

06Four questions to ask when looking at a parameter table

item Question Points I want to confirm
1 Is ε 'given together Only looking at μ cannot determine whether impedance matching is feasible
2 Is the filling method volume fraction or weight fraction The difference between the two is significant, and mixing them can lead to misjudgment
3 Has the sample undergone orientation treatment The orientation of μ 'is not on the same order of magnitude
4 Is there a corresponding transition at the peak of μ ' Use causality to screen out suspicious data

The technological threshold for magnetic medium absorbing materials lies in converting the potential of powder into the actual medium. The fact that the same batch of powder can produce products with significant differences indicates that there is no standard answer to this matter, and it is precisely where the formula and process are truly valuable.

For more technical information on magnetic absorbing materials, magnetic absorbing plates, and effective medium design, please visitwww.avanzado.cn.

Contact

Contact us

Company:Xianjin Yuan (Shenzhen) Technology Co., Ltd.

Address: 8/F, Zhongxing Building, Shajing Xinsha Road, Bao'an District, Shenzhen, Guangdong, China

Tel: 0755-22277778   13826586185

Email: duanlian@xianjinyuan.cn

Hotline
0755-22277778
13826586185(Mr.Duan)
Wechat QRcode Wechat QRcode